“After retorting at 121°C for 30 minutes, bubbles appeared along the edges of the packaging bag, followed by interlayer delamination. The layers could be peeled apart with little effort.”

This is one of the most common quality issues reported by users of PVDC composite films. Retort delamination affects more than just the appearance of the package. It can directly compromise the integrity of the barrier layer, significantly shortening the product's shelf life. Even more frustrating, replacing the adhesive with a higher-strength grade or increasing the adhesive coating weight may still fail to eliminate the problem.

So, where does the root cause actually lie?

1. The Root Cause of Retort Delamination: The Balance Between Shrinkage Stress and Bond Strength

PVDC composite films typically feature a multilayer structure, with PVDC serving as the intermediate barrier layer and being laminated to substrates such as BOPA, BOPET, and CPP using an adhesive. During high-temperature retorting at 121°C, all layers undergo thermal shrinkage, but their shrinkage rates can differ significantly. This difference is one of the fundamental causes of delamination.

PVDC is a thermally sensitive film with a relatively high thermal shrinkage rate. Taking Dow Chemical's Saran 2032 film as an example, shrinkage begins at room temperature around 30°C. After three minutes in 100°C hot water, shrinkage can reach approximately 28%–30% in the machine direction and 22%–24% in the transverse direction. Under retort conditions at 121°C, the shrinkage of the PVDC layer can become even more pronounced.

As the PVDC layer attempts to shrink significantly, the adhesive layer must withstand the substantial shear stress generated by this shrinkage. If the initial tack and ultimate bond strength of the adhesive are insufficient to withstand this stress, interlayer delamination can occur.

An even less obvious issue is that PVDC may already have been stretched during the lamination process. If lamination tension is not properly controlled, the PVDC layer may remain in a “pre-stretched” state after lamination. During retorting, the stored internal stress is released, significantly increasing the risk of delamination.

In addition, uneven PVDC thickness can lead to an uneven distribution of shrinkage stress. Thinner areas are subjected to greater localized stress concentrations and are therefore more susceptible to localized delamination after retorting.

Therefore, the fundamental mechanism behind retort delamination is the interaction between PVDC shrinkage stress and interlayer bond strength. The bond strength must remain sufficiently higher than the shrinkage stress generated during retorting.

PVDC resin.png

2. Solution One: Select a Retort-Resistant Adhesive

When selecting an adhesive, both solvent-based and solvent-free systems have their own suitable applications.

Solvent-based polyurethane adhesives generally provide higher initial tack and are suitable for high-speed lamination lines and applications with demanding initial bond-strength requirements. However, they face increasing compliance pressure related to solvent residues and VOC emissions.

Solvent-free adhesives eliminate solvent residue issues and represent an important direction for the industry. However, their initial tack is generally lower than that of solvent-based adhesives, making them more demanding in terms of tension control and curing conditions.

For PVDC composite films used in retort applications, retort-resistant solvent-free adhesives should be evaluated as a priority. However, suppliers should be asked to provide actual peel-strength data under 121°C retort conditions, and complete retort validation should be performed before mass production.

A retort-resistant solvent-free adhesive typically has three key characteristics.

First
Sufficient initial tack. The adhesive should form an effective bond shortly after lamination to prevent the PVDC layer from shifting before curing is complete.
Second
High ultimate bond strength. Through a high crosslinking-density design, the adhesive should retain sufficient peel strength even after retorting at 121°C.
Third
Excellent hydrolysis resistance. During retorting, the penetration of water vapor should not cause degradation of the adhesive layer.
3. Solution Two: Optimize Lamination Tension and Process Compatibility

Even with the right adhesive, retort delamination cannot be effectively eliminated if the lamination tension and process parameters are not properly matched.

3.1 Lamination tension control is critical.

During lamination, the PVDC layer should be maintained at relatively low tension to minimize pre-stretching.

The unwinding tension should be kept relatively low, while the winding tension should use a decreasing taper-tension design to prevent excessive internal pressure from causing creep in the PVDC layer.

The exact values vary depending on the equipment, substrate, and film width. However, the basic principle is that the unwinding tension of the PVDC layer should be lower than that of the other substrates, and the winding tension should generally not exceed 1.2 times the unwinding tension.

It should be noted that actual tension settings are highly dependent on the equipment model, film width, substrate type, and line speed. The above values are provided for reference only.

3.2 Adhesive coating weight and lamination temperature must be properly matched.

For solvent-free adhesives, the coating weight is typically controlled at approximately 1.2–1.8 g/m². For retort applications, it can be appropriately increased to 1.5–2.0 g/m².

If the coating weight is too low, the adhesive layer may fail to form a continuous bond. If it is too high, excessive adhesive thickness may instead lead to internal stress concentration.

The recommended lamination temperature is generally 40–50°C. If the temperature is too low, adhesive flowability may be insufficient. If it is too high, premature shrinkage of the PVDC layer may occur.

Lamination pressure should be sufficient to ensure close contact between the layers, but excessive pressure should be avoided to prevent damage to the PVDC barrier layer.

3.3 The curing process should not be overlooked.

Solvent-free adhesives are typically cured at 40–50°C for 24–48 hours.

Insufficient curing can result in inadequate crosslinking of the adhesive and insufficient bond strength during retorting. Excessive curing time, on the other hand, may reduce production efficiency.

It is recommended to follow the process conditions specified by the adhesive supplier and conduct retort testing on samples after curing.

3.4 PVDC layer thickness uniformity is equally important.

Uneven PVDC thickness can result in an uneven distribution of shrinkage stress. Thinner areas are exposed to greater localized stress concentrations and are therefore more likely to develop localized delamination after retorting.

The thickness deviation of the PVDC layer should be controlled within ±5%.

For coated PVDC composite films, uniformity of the coating weight directly affects thickness distribution. For co-extruded PVDC composite films, die design and extrusion stability are critical factors.

It is recommended to add PVDC layer thickness uniformity to the incoming-material inspection program and to pay close attention to the effect of thickness variation on retort delamination during lamination process trials.

4. Solution Three: Optimize the Film Structure

In addition to adhesive selection and process control, film structure design also affects the risk of retort delamination.

When designing the film structure, the selection of tie or transition layers requires careful evaluation.

EVA is a well-established transition-layer material for low-temperature refrigeration and heat-shrink packaging applications. However, its temperature resistance is limited. EVA films are typically used below 80°C. Under retort conditions at 121°C, the EVA layer may soften or even degrade, potentially becoming a new weak point for delamination.

For retort applications, the transition layer should be made from a temperature-resistant polyolefin elastomer or a modified EVA grade with appropriate heat resistance, ensuring that it does not soften or degrade under 121°C conditions.

During the film structure design stage, it is recommended to systematically evaluate the temperature resistance of every layer and ensure that differences in thermal shrinkage between layers remain controllable at retort temperatures.

Selecting a heat-sealing layer with a shrinkage rate closer to that of PVDC can also help reduce stress differences between layers.

5. Frequently Asked Questions (FAQ)
Q: Why does retort delamination still occur after switching to a retort-resistant adhesive?

The adhesive is only one of the variables involved. Retort delamination is a manifestation of a systematic process issue.

If tension control is inadequate, the PVDC layer may already be pre-stretched during lamination. When the package is retorted, the stored shrinkage stress is released in a concentrated manner, making it difficult to withstand even with a high-strength adhesive.

It is recommended to check whether the unwinding and winding tensions are properly matched and to confirm whether the curing process is sufficient.

If delamination occurs during the cooling stage after retorting, it is generally necessary to investigate two possible causes: insufficient hydrolysis resistance of the adhesive or an excessively rapid cooling rate.

Q: Can solvent-free lamination always solve PVDC retort delamination?

Solvent-free lamination eliminates solvent residues and avoids the thermal shock to the PVDC layer caused by a high-temperature drying oven, making it a more favorable processing route.

However, solvent-free adhesives generally have lower initial tack than solvent-based adhesives and therefore place higher demands on tension control and curing conditions.

If the tension-control system of the equipment does not provide sufficient accuracy, or if the curing conditions do not meet the required specifications, delamination can still occur with solvent-free lamination.

Before mass production, it is recommended to conduct complete retort validation tests under both 121°C/30 minutes and 121°C/40 minutes conditions.

Test samples should be taken separately from the seal area, middle section of the bag body, and folded corners, with the lowest measured value used as the basis for evaluation.

Q: What peel strength is considered acceptable for PVDC composite film after retorting?

The industry generally requires a peel strength of no less than 4.0 N/15 mm after retorting at 121°C for 30 minutes, with reference to the requirements for retort-resistant products in GB/T 10004, Plastic Composite Film and Bags for Packaging.

For products that need to withstand retorting at 121°C for 40 minutes, a target value of at least 5.0 N/15 mm is recommended.

It should be noted that both the peel-strength test method and sampling location can affect the results. It is recommended to take samples separately from the seal area, middle section of the bag body, and folded corners, and use the lowest measured value as the basis for evaluation.

Conclusion

The retort delamination problem in PVDC composite films is essentially a balance between the thermal shrinkage characteristics of the materials and the bond strength between layers.

The solution does not lie in simply “upgrading” a single material. Instead, it requires systematic coordination among adhesive selection, lamination tension control, curing conditions, film structure design, and thickness uniformity.

1
Selecting a retort-resistant solvent-free adhesive with sufficient initial tack and ultimate bond strength is the first step.
2
Optimizing lamination tension and process parameters to prevent the PVDC layer from being pre-stretched is the second step.
3
Conducting retort validation tests and continuously refining the process based on the test results is the third step.

Only by implementing all three steps systematically can the high-barrier performance of PVDC be fully realized in high-temperature retort packaging applications.

Erik

Sales Manager
I'm a Sales Consultant at TPS Chemical with over 10 years of experience in the chemical and plastics industries. I specialize in providing clients with professional and reliable material solutions. With a deep understanding of product applications, market demands, and supply chains, I am dedicated to helping clients enhance formulation value and explore more efficient and sustainable application opportunities.